河北鋼邊橡膠止水帶熱熔機焊接時的步驟分幾步走?
鋼邊橡膠止水帶熱熔機焊接時的步驟分幾步走?衡水融通橡膠制品有限公司在工程施工中,經常要用到鋼邊橡膠止水帶,一般默認鋼邊橡膠止水帶的長度是一卷20米,但是在實際應用中,這個長度不一定比較合適,那么就需要對鋼邊橡膠止水帶進行切割和焊接來使用,保證施工的正常進行。鋼邊橡膠止水帶焊接需要用到止水帶熱熔焊機,熱熔焊機分為模具和控制箱兩部分組成,如何進行鋼邊橡膠止水帶的焊接呢?

鋼邊橡膠止水帶熱熔機焊接時的步驟分幾步走?
Hengshui Rongtong Rubber Products Co., Ltd. often uses steel-edged rubber water stops in engineering construction. Generally, the default length of steel-edged rubber water stops is a roll of 20 meters, but in practical application, this length is not necessarily appropriate, so it is necessary to cut and weld steel-edged rubber water stops to ensure the normal construction. Welding of steel-edged rubber water-stop strip requires hot-melt welding machine with water-stop strip. The hot-melt welding machine consists of die and control box. How to weld steel-edged rubber water-stop strip?
需要焊接的鋼邊止水帶規格要符合要求并且檢驗合格,其次需要焊接的環境不能被雨淋暴曬,也不能接觸污染性較強的化學物質。
1、將鋼邊橡膠止水帶需要搭接的部分做好標記,保證中間能夠塞進1cm左右的生膠片。
2、用切割機切割鋼邊橡膠止水帶中間的橡膠,需要切30cm左右,注意不要切到鋼邊,然后用角磨機打磨需要搭接的橡膠部分。

鋼邊橡膠止水帶熱熔機焊接時的步驟分幾步走?
3、裁剪兩條生膠片堵住鋼邊止水帶的中間圓孔不分,長度不少于5cm。
4、需要將鋼邊進行鉚釘,用手鉆在鋼邊上打眼,固定搭接的鋼邊止水帶的鋼邊部分。
5、將預熱好的熱熔機的熱硫化夾具墊在需要搭接的鋼邊止水帶下,填充好生膠片。
6、安裝好夾具放置千斤頂,控制熱熔機溫度在130-150攝氏度之間,同時用千斤頂加壓,保證夾具與鋼邊止水帶面貼合緊密,大概20分鐘后取下夾具即可。